Table-1: Unsaturated polyester Resin System (General Purpose)
Polyester resin 100 parts by mass
styrene monomer (optional) 5 parts by mass
Cobalt octoate accelerator (1 %) 0.5 parts by mass
Cumene hydroperoxide 1.5 parts by mass
Impregnation temperature As specified by manufacturer
Cure 16 h at 110 °C
Table-2: Another Unsaturated Polyester Resin System (General Purpose)
Polyester resin 100 parts by mass
Benzoyl peroxide 2 parts by mass
Impregnation temperature As specified by manufacturer
Cure 16 h at 110 °C
Table-3: Epoxy Resin (MTHPA Hardener: Acid Anhydride System)
Epoxy resin 100 parts by mass
Methyltetrahydrophthalic acid anhydride (MTHPA) 80 parts by mass
N, N-dimethylbenzylamine 1 part by mass
Impregnation temperature 40 °C
Cure 16 h at 120 °C

Inquiry for Our Product

YuanBo Engineering Co., Ltd.
E-mail: angela@yongber.com

When you contact us, please provide your detail requirements. That will help us give you a valid quotation.

Full Name *
Country Code * + Phone Number *
Message *